14指状凹陷14指状凹陷
14 Localised, glossy, finger-shaped depressions
14 局部的光泽指状凹陷
Alternative terms: "Tacky spots"
别名, 粘性斑点
Description: Glossy depressions, often near the sprue, at cores or in
the vicinity of hot runner units
描述, 光泽凹陷,通常出现在流道、型芯或热流道单元附近
Possible causes:...
14指状凹陷
14 Localised, glossy, finger-shaped depressions
14 局部的光泽指状凹陷
Alternative terms: "Tacky spots"
别名, 粘性斑点
Description: Glossy depressions, often near the sprue, at cores or in
the vicinity of hot runner units
描述, 光泽凹陷,通常出现在流道、型芯或热流道单元附近
Possible causes: 1 Holding pressure ineffective
2 Switch from injection to holding pressure made too
soon
3 Mould temperature too high in places
4 Cooling time too short
可能的原因, 1 保压压力无效
2 注射到保压的切换太早
3 局部的模具温度太高
4 冷却时间太短
Remedial actions: 1 Increase holding pressure and holding pressure time
2 Switch to holding pressure at a later stage
3 Reduce mould temperature locally by means of
additional cooling channels or separate temperature
control
4 Extend cycle time
解决的措施, 1 增大保压压力和延长保压时间
2 推迟注射到保压的切换
3 通过增加额外的冷却流道或采用独立的温度控制来降低局部
的模具温度
4 延长冷却时间
Notes: See also 02 (Matt surface defects...) 注释, 参看02 (消光
面缺陷)
Fault category: Gloss / Surface irregularities 缺陷类别, 光泽、表面不规则
本文档为【14指状凹陷】,请使用软件OFFICE或WPS软件打开。作品中的文字与图均可以修改和编辑,
图片更改请在作品中右键图片并更换,文字修改请直接点击文字进行修改,也可以新增和删除文档中的内容。
[版权声明] 本站所有资料为用户分享产生,若发现您的权利被侵害,请联系客服邮件isharekefu@iask.cn,我们尽快处理。
本作品所展示的图片、画像、字体、音乐的版权可能需版权方额外授权,请谨慎使用。
网站提供的党政主题相关内容(国旗、国徽、党徽..)目的在于配合国家政策宣传,仅限个人学习分享使用,禁止用于任何广告和商用目的。